招锦健 刘崇志 朱健
【摘 要】某核电站大修发现,给水泵组增压泵泵轴与机械密封轴套配合处有不同程度的腐蚀,存在设备可靠性隐患。通过理论分析和现场检查确认腐蚀现象为缝隙腐蚀,对缝隙腐蚀形成机理进行分析,并提出改进措施防止腐蚀再次发生。
【Abstract】In the overhaul of a nuclear power plant, it is found that there is varying degrees of corrosion in the joint of the booster pump shaft and mechanical seal sleeve of the feed water pump unit, and there is hidden danger of equipment reliability. Through theoretical analysis and on-site inspection, the corrosion phenomenon is confirmed as crevice corrosion. The formation mechanism of crevice corrosion is analyzed, and the improvement measures are put forward to prevent the corrosion from happening again.
【关键词】给水泵;泵轴;缝隙腐蚀
【Keywords】 feed water pump; pump shaft; crevice corrosion
【中图分类号】TK223 【文献标志码】A 【文章编号】1673-1069(2018)11-0145-02
1 引言
在某核电站1、2号机组大修中发现,增压泵泵轴在与机械密封轴套配合处发现不同程度的腐蚀,腐蚀发生的位置沿轴向宽带分布,圆周向不连续,对应机械密封轴套O形密封圈密封处的空气侧。大修中采取外送泵轴激光熔覆和现场微弧焊对泵轴腐蚀处进行修复,修复后对泵轴进行圆滑打磨,避免回装机械密封后在轴套O 形密封圈处发生泄漏。分析该腐蚀现象的形成机理,防止类似现象再次发生。
2 设备简介
泵轴材料为UNS S42000马氏体不锈钢,化学成分为:w(C)≤0.15%、w(Si)≤0.1%、w(Mn)≤0.1%、w(P)≤0.04%、w(S)≤0.03%、12%≤w(Cr)≤14%。机械密封轴套材料为316不锈钢,机械密封动环通过轴套与轴固定,轴套通过轴套锁母與泵轴固定,机封轴套与轴为间隙配合。轴套内部设有O形密封圈,用于防止泵内介质从轴套处泄漏。O形密封圈材质为三元乙丙橡胶(EPDM),规格为130.00 mm×3.53 mm。密封圈槽为矩形槽,尺寸为深3 mm、宽5 mm。
3 故障现象及初步分析
3.1 故障现象
某核电站1号机组第7次大修中3号增压泵解体检查发现,泵轴两端安装机械密封轴套O形密封圈处空气侧表面腐蚀,1号增压泵的泵轴非驱动端安装机械密封轴套O形密封圈处空气侧表面也存在腐蚀。……