洪新阳 徐斌
摘 要:文章针对农业机械使用的渐开线内花键齿轮,在热处理渗碳淬火中内花键易产生轴向锥度、M值超差、塞规不过等现象,对本公司生产的内花键齿轮进行原材料、锻造正火、拉花键、热处理的各环节多次试验,然后通过数据分析、归纳总结、工艺改进,对齿轮内花键变形的产生原因进行分析,并采取工艺措施进行控制,从而提升产品质量。
关键词:内花键;渗碳淬火;锥度
中图分类号:TG162.73 文献标志码:A 文章编号:2095-2945(2018)11-0090-03
Abstract: In this paper, for involute internal spline gears used in agricultural machinery, the internal splines easily produce such phenomena as axial taper, M value excess difference and plug gauge in heat treatment of carburizing and quenching. The internal spline gear produced by our company has been tested for many times in raw materials, forging normalizing, drawing spline and heat treatment. Then, through data analysis, induction and process improvement, the causes of distortion of inner spline in gear are analyzed. And take the process measures to control, so as to improve the quality of products.
Keywords: internal spline; carburizing and quenching; taper
1 内花键齿轮技术参数与加工工艺
1.1 内花键齿轮的技术参数及结构
齿轮内花键参数:模数:m=1.25、齿数:z=30、压力角:α=20°、大径:D=40、大径:d=37.5、量棒直径:dp=2.61、跨棒距直径:M=34.657-34.753、材料:20CrMnTi、热处理:渗碳淬火S0.7~C59。
1.2 加工工艺
锻造→正火→粗车→拉花键→精车→切齿→渗碳淬火→研磨配对。
2 工艺改进前产品质量情况
目前农业机械中,也广泛使用了同步器结构,如大中型拖拉机,这样渐开线内花键齿轮结构越来越多,而这类齿轮由于结构较复杂、不对称、壁厚较薄,在热处理渗碳淬火后,造成齿轮内花键跨棒距M值超差,内花键产生较大的轴向锥度,综合塞规不能通过,造成装配困难等问题。由此客户质量抱怨较多,甚至要求质量索赔。
(图1)齿轮工艺改进前内花键检测结果为:跨棒距M值最大缩量为0.13mm,内花键轴向锥度为0.10mm,综合塞规通过率为50%。
3 齿轮内花键热处理变形原因分析
影响齿轮内花键变形的因素很多,有原材料、锻造与正火工艺、冷加工拉花键工艺、热处理工艺等方面。
3.1 原材料对齿轮内花键变形的影响……p>