XU Chengliang, TENG Huaxiang, JIANG Guangrui, LI Yan, LI Min, LIU Guanghui
(Shougang Research Institute of Technology, Shougang Group Co., Ltd, Beijing 100043, China)
Abstract: The solidification and corrosion behavior of the Ti/B added Zn-Al-Mg alloys were experimentally investigated by means of microstructure characterization and electrochemical test. The basic calculations were carried out to predict the characteristics of the Ti-added Zn-Al-Mg alloys. The Zn-Al-Mg ingots with minor doping of Ti/B were prepared and solidified under different cooling rate, including air cooling, water quenching and furnace cooling. The scanning electron microscopy (SEM) and the X-ray diffraction method (XRD) were used to determine the microstructures and phase types of the alloy samples. It could be discovered that trace TiAl3 particles were dispersed in the Ti/B added alloy samples which provide the heterogeneous nucleation sites to refine the size of the dendrites and the eutectic microstructures. More fined microstructures with the addition of both Ti and B were obtained compared with those with the merely addition of Ti, and the water cooled alloys presented the finest microstructures due to the fastest cooling rate. It could also be noticed that with the increasing solidification rate, the percentage of the MgZn2 phase turned out to be higher because of the Mg2Zn11↔MgZn2 transition, which is in consistent with the results in the actual hotdip galvanizing process. Electrochemical experiments in the previous work included methods the of the Tafel polarization test and the electrochemical impedance spectroscopy test (EIS). Results show that the quenched Zn-Al-Mg alloy with the addition of both Ti and B takes on best corrosion resistance. Consequently, the addition of certain amount of Ti/B elements and the appropriate elevation of the cooling rate will be the practicable approaches to optimize the microstructure and the corrosion resistance of the Zn-Al-Mg coatings in the actual galvanizing process.
Key words: Ti/B added Zn-Al-Mg alloy; cooling rate; solidification; corrosion resistance
et al
investigated the effect of Ti addition on the multiphase microstructure of the Zn-Al-Mg coating, and discovered that the eutectic microstructures were more obvious because of the Ti-based surface activation. Chenet al
studied the constitution of the Fe-Al layer of the Zn-6%Al-3%Mg coating, and confirmed that the addition of Ti will improve the qualities of the intermetallic alloy layers. Hondaet al
discovered that with the addition of Ti, the precipitated TiAlphase will provide the heterogeneous nucleation sites for the growth of the primary and eutectic solidified phases and refine the microstructures of the Zn-Al-Mg alloys. Furthermore, when a trace amount of B is added in the Ti-included Zn-Al-Mg alloy coatings, the refinement of the microstructures will become more obvious, and the micro-hardness and the wearing qualities will be further enhanced on the basis of the research by Wanget al
.The cooling rate of the galvanized coatings is significant concerning the microstructures and the corrosion resistance of the coated products. Kimet al
analyzed the dendritic morphologies and the related growth directions in the galvanized Zn-0.2%Al coatings, but the effect of cooling rate on the solidified microstructures was not discussed in their research. Elvinset al
studied the influence of solidification rate on the microstructure and corrosion resistance of Zn-4.5%Al coating, and discovered that with the increase of cooling rate, the primary phases in the coating were further refined, which resulted in the decrease of the corrosion resistance. However, this conclusion may have academic dispute based on the corrosion theory. So according to the available literature reports, the fundamental study concerning the solidification processes and the related corrosion behaviors of the Ti/B added Zn-Al-Mg alloys caused by different cooling rate are relatively scarce. Motivated by the corresponding achievements concerning the small amount of element-doping method in the Zn-Al-Mg alloy coatings, the present work was intended to systematically investigate the solidification rate and the corrosion behavior of the Ti/B added Zn-Al-Mg alloys, which will provide fundamental guidance to the practical manufacturing processes of the galvanized coatings.Zn(99.99wt%), Al(99.99wt%), Zn-11wt%Mg, Al-10wt%Ti, and Al-8wt%B alloys were used as raw materials. Thereinto, the Zn-11wt%Mg were selected as master alloy in case of the drastic oxidation of Mg in the melting process. For Ti and B, it could be discovered that these two elements are prone to form high melting point compounds during the melting process, and the use of master alloys of Ti and B could significantly decrease the burning loss rate. The alloy samples were prepared by the high frequency induction furnace under the protection of Ar. Firstly, the zinc ingots were added in the in the furnace, and the furnace temperature increased to 600 ℃ at the speed of 10 ℃/min. When the zinc ingots melted completely, the aluminum ingots and the Zn-11wt%Mg master alloys were added in the furnace subsequently. The Al and Zn-11wt%Mg should be pressed and melted under the surface of molten Zn using a graphite hood to ensure the complete melting of these low-density alloys. Then, the Al-10wt%Ti and Al-8wt%B were added in the similar way in order to obtain the homogenous compositions of the Ti/B contained Zn-Al-Mg alloys. Finally, the furnace was cooled to room temperature in different cooling rate, including water quench, air cooling and furnace cooling, respectively. For the water quenched alloy samples, the samples were poured in the copper mould displayed in a water recycling system. For the air cooling alloy samples, the samples were poured in the AlOmould and cooled in the air. For the furnace cooling alloy samples, the samples were displayed in the furnace and slowly cooled to room temperature.
The cooled alloy samples were then processed intoφ
20 mm×1 mm plates for SEM, XRD, and electrochemical experiments. The PARSTAT 2273 electrochemical workstation were applied to conduct the Tafel polarization test and the EIS test. The concentration of 3.5wt% NaCl solution was selected as the electrolyte and the test temperature was 30±2 ℃. The three-electrode system was used in the experimental process, with Pt as the counter electrode, saturated calomel as the reference electrode (SCE), alloy samples as the working electrode, respectively. When measuring the Tafel polarization curves of the alloy samples, the scanning rate and scale of the electric potential was set as 1 mV/s and -1.25 - -0.75 V (vs
SCE) to obtain the required strong polarization region of the electrochemical test. When dealing with the measurement of the EIS, the amplitude of the AC signal was set as 10 mV, and the measurement scale of the AC frequency was 10-10Hz to fully reflect the characters of the EIS curves in both the high and low frequency regions. Before the electrochemical test, all the alloy samples were placed in the 3.5wt% NaCl solution for 2 h in order to get the stable surface available for the experiment.3.1.1 The solidification process calculations of the Ti added Zn-Al-Mg alloys
The experimental studies of the microstructures and the morphologies of the Zn-based coated alloys are relatively abundant. Ahmadiet al
investigated the grain refinement on the microstructure and the related cracking resistance of the Zn-Al-Mg coatings by Electron backscatter diffraction. Hatet al
discussed the effect of Sb addition on the Zn-Al-Mg alloys, and discovered that with the addition of 0.3wt% Sb, the Zn-Al-Mg alloys take on an excellent corrosion resistance. Grandhiet al
studied the effect of Mn addition on the galvanized zinc coating, and found that the addition of 1.2wt% Mn will benefit the related appearance, morphology and corrosion resistance of the alloy coating. From the recent literature reports, it could be noticed that the basic theories of the solidification process concerning the Ti/B added Zn-Al-Mg alloys were not fully analyzed. Particularly, the precipitation temperatures of the TiAl, Al-rich phases, MgZn, Zn-rich phases and the corresponding phase fractions of the Ti-added Zn-Al-Mg alloys were not reported in previous literatures, and these basic thermophysical properties are important to predict and design the suitable hot-dip parameters. In this work, the thermodynamic calculations were carried out for compositions Zn-6%Al-3%Mg and Zn-6%Al-3%Mg-0.1%Ti respectively, and the calculation results are shown in Fig.1. It is predicted that with a small addition of Ti, the TiAlphase will precipitate at the temperature of 620 ℃ during solidification process. According to the related literature reports, the trace amount of TiAlparticles act as the heterogeneous nucleation sites which will contribute to the formation of the refined grains in the solidified microstructures. Thus, the Ti-added Zn-Al-Mg coatings may possess better corrosion resistance than the Zn-Al-Mg coatings, and the dispersed TiAlparticles will play a vital role in the grain refinement of the coat structures. The thermodynamic calculation well predicted the precipitation temperatures and the precipitation phases of the Ti-added Zn-Al-Mg alloys, which will provide reliable reference data for the practical galvanized process.
Fig.1 The thermodynamic calculation results of the Zn-6%Al-3%Mg and Zn-6%Al-3%Mg-0.1%Ti compositions: (a) Solidification curve of the Zn-6%Al-3%Mg composition; (b) Temperature-mass fraction relationship of the Zn-6%Al-3%Mg composition; (c) Solidification curve of the Zn-6%Al-3%Mg-0.1%Ti composition; (d) Temperature-mass fraction relationship of the Zn-6%Al-3%Mg-0.1%Ti composition
3.1.2 The DFT calculations of the TiAlphase and the interface stability prediction of the TiAl/Al and TiAl/Zn phase boundaries
As mentioned above, the TiAlparticles act as the heterogeneous nucleation sites in the solidification process of the Ti-added Zn-Al-Mg coatings. Besides, D0-TiAlphase is more stable than L-TiAlphase, and D0-TiAlphase was observed in the alloy coatings according to the related literature reports. However, the amount of the TiAlphase is quite small in the Zn-Al-Mg coatings, so it is difficult to experimentally measure the compatibility and the hardness of the Ti-added Zn-Al-Mg coatings. In order to justify the practicability of the Ti addition in the zinc pot during the actual galvanizing process of the Zn-Al-Mg coatings, the density functional theory (DFT) calculations were carried out to quantitatively predict the metallicity and the wearing qualities of the Tiadded Zn-Al-Mg coatings.
In this work, the generalized gradient approximation (GGA) method was adopted to describe the exchange and correlation potential functionε
[ρ
(r
)]. For the selection of the pseudo potential function, the Perdew-Burke-Ernzerhof (PBE) function was used based on the Projector-Augmented-Wave (PAW) plane wave method. The cut-off energy was set as 310 eV, and the convergence precision was ultra-fine to ensure the accurate calculation results. The k-points were divided into 6×6×3, and the calculation precision was set Fine accounting for both the calculation efficiency and the calculation precision.Before the calculation work, the crystal structure of D0-TiAlphase was reviewed from the previous literatures. It is reported that the D0-TiAlphase (a
=0.3850,c
=0.8584 nm) takes on body-centered tetragonal structure with the space group I4/mmm. The atomic site occupations of D0-TiAlphase are Ti (0.00, 0.00, 0.00), Al (0.00, 0.00, 0.50), and Al (0.00, 0.50, 0.25). Then, using the DFT calculation method, the calculated band structure and the density of states (DOS) are shown in Fig.2, and the elastic constants of both D0-TiAland Hcp_Zn are listed in Table 1 as a comparison. From the calculation results, it could be noticed that D0-TiAlphase has prominent metallic property, for there is no obvious band gap from both the calculated band structure and the density of states. Consequently, with the fine metallicity, the D0-TiAlphase has well compatibility with the molten zinc, which will less likely form the impurities or defects on the surface of the alloy coatings. Moreover, the D0-TiAlphase possesses higher Bulk modulus compared with Zn, which means the existence of trace D0-TiAlphase will contribute to the hardness and stiffness of the alloy coatings. As a result, the Ti-added alloy coatings will take on excellent wearing qualities.
Fig.2 The DFT calculation results of the D022-TiAl3 phase: (a) The crystal structure; (b) The calculated band structure; (c) The calculated density of states (DOS)
Table 1 The calculated elastic constants of D0-TiAl phase and Hcp_Zn
Phases The elastic constants Cij/GPa Bulk modulus/GPa D022-TiAl3 C11=180.17 C12=94.84 C13=40.68 C33=204.78 C44=39.42 C66=121.73 101.57±0.599 Zn C11=206.33 C12=34.90 C13=-17.08 C33=39.91 C44=-30.59 C66=85.71 23.23±2.823
In order to further predict the heterogeneous nucleation site of the TiAlincluded Zn-Al-Mg alloy coatings, the DFT calculation was carried out to find out the interface stabilities of the TiAl/Al and TiAl/Zn. According to previous reports, the growth planes and directions for TiAl(200)[010] and Al(200)[010] will take on low lattice disregistry, which means the Al(200)[010] crystal is prone to nucleate heterogeneously on TiAl(200)[010]. Moreover, both the TiAland Al are cubic structures, so the lattice matching is relatively fine for the Al phase growing epitaxially on the TiAlparticles. For TiAl(200)[010] (1×1) / Al(200)[010] (1×2) interface model, the lattice disregistry is < 5%, so this orientation was adopted in this work, and the interface area A is 3.95×8.38 Åfor this model. In terms of TiAland Zn, the TiAlphase is cubic structure while the Zn phase is the hexagonal close-packed structure, thus the lattice disgregistry is relatively significant which will hinder the crystal growth. For the orientation of TiAland Zn, it is reported that the hexagonal (1120) plane has the low lattice disregistry with the cubic (100) plane. To facilitate the construction of the required surface model, the hexagonal Hcp_Zn phase was converted to the orthogonal style, and the supercell model was utilized to obtain the optimum lattice matching. In this work, the lattice disregistry is < 5% for TiAl(200)[010] (5×2) / Zn(110)[001] (4×3) interface, and the interface area A turns out to be 19.22×16.77 Å. The interface model of TiAl/Al and TiAl/Zn is displayed in Fig.3, and the calculated surface energies are listed in Table 2. The corresponding formula used for calculating the surface energies is:

Fig.3 The interface models of the D022-TiAl3(200)/Al(200) and D022-TiAl3(200)/Zn(110)
Table 2 The values of the corresponding interfacial energies
Interface Area/Å2Interfacial energies/(eV/ Å2)D022-TiAl3(200)/Al(200) 33.1 -1.027×10-1 D022-TiAl3(200)/Zn(110) 322.3 3.289×10-2

Fig.4 The microstructures and XRD patterns of the quenched Ti/B added Zn-Al-Mg alloys: (a) The microstructure of the quenched Zn-6%Al-3%Mg-0.1%Ti; (b) The microstructure of the quenched Zn-6%Al-3%Mg-0.1%Ti-0.05%B; (c) The XRD patterns of the quenched alloys

Fig.5 The microstructures and XRD patterns of the air cooled Ti/B added Zn-Al-Mg alloys: (a) The microstructure of the air cooled Zn-6%Al-3%Mg-0.1%Ti; (b) The microstructure of the air cooled Zn-6%Al-3%Mg-0.1%Ti-0.05%B; (c) The XRD patterns of the air cooled alloys

E
represents the energies of the interface structures (E
=-7 765.3 eV andE
=-217 206.2 eV),E
andE
represent the total energies of the single planes (E
=-708 8.7 eV andE
=-673.2 eV,E
=-53 121.2 eV, andE
=-164 095.6 eV, respectively). From the calculation results, it could be noticed that the surface energy of the TiAl/Zn interface turns out to be a slight positive value, although the supercell models are used to lower the lattice disregistry. Consequently, the TiAl/Al interface should be more stable than the TiAl/Zn interface, and the Al phase will precipitate on the TiAl(200) interface preferentially. The calculated results further predicted the possible SEM morphologies presented in the following section.The solidification processes of Zn-6%Al-3%Mg-0.1%Ti and Zn-6%Al-3%Mg-0.1%Ti -0.05%B alloys were experimentally conducted by means of water quenching, air cooling and furnace cooling. Figs.4-6 present the microstructures and the XRD patterns of the alloys samples with different cooling method. It could be noticed that the quenched alloys possess the finest grain size, and the morphologies of the quenched microstructures are very close to those of the practical manufactured Zn-Al-Mg alloy coatings. It is also apparent that the quenched alloys possess the most eutectic microstructures and the least primary Fcc_Al phases. The TiAlparticles mostly distribute in the primary Fcc_Al phase according to the SEM microstructures in Figs.4 and 5, which is also supported by the DFT calculation results in Section 3.1. It should be noticed that for the furnace cooled alloy samples, the existence of TiAlparticles could be hardly observed. The reason may lie on that the high-melting TiAlphase will not nucleating in the molten alloys because of the slow cooling rate, but entering into the floated slags during the solidification process. As a result, the addition of Ti/B will not markedly contribute to the refinement of the furnace-cooled microstructures.

Fig.6 The microstructures and XRD patterns of the furnace cooled Ti/B added Zn-Al-Mg alloys: (a) The microstructure of the furnace cooled Zn-6%Al-3%Mg-0.1%Ti; (b) The microstructure of the furnace cooled Zn-6%Al-3%Mg-0.1%Ti-0.05%B; (c) The XRD patterns of the furnace cooled alloys
The cooling rate also plays a vital role in the existence form of the Mg-Zn compounds,i e
, MgZnor MgZnin the solidified microstructures. Menget al
and Kimet al
studied the crystal structures and the phase morphologies of MgZnand MgZncompounds. Maet al
and Sullivanet al
discovered that there exist a isomeric transition MgZn↔MgZnin the practical solidification process of the Zn-Al-Mg alloy. In both the SEM graphs and the XRD patterns of the quenched and the air cooled alloy samples in the present work, it could be discovered that there exist the MgZn/MgZnmixed phases in the solidified microstructures. For the furnace cooled alloy samples, however, only the MgZnphase could be discovered in the solidified microstructures. With the increase of the cooling rate, the existing MgZnphase will be prone to change into MgZnphase. This phenomenon is further supported by the fact that the produced Zn-Al-Mg galvanized coatings possess the vast majority amount of MgZnphase because of the fast cooling rate in the practical galvanized process. Also, it was reported that due to the rapid solidification process, the MgZnphase possesses higher nucleation rate than MgZnphase in the supercooled liquid. As a result, the stable MgZnphase (primitive-cubic structure with space groupPm3
) will transfer into the metastable MgZnphase (hexagonal structure with space groupP6mmc
) if the cooling rate exceeds a certain extent. Consequently, it is important to obtain the appropriate cooling rate to assure the optimum grain size available for the required corrosion resistance of the Zn-Al-Mg coatings.The Tafel polarization curves and the electrochemical impedance spectroscopy (EIS) curves were experimentally measured by the aforementioned electrochemical workstation. The polarization curves of the Ti/B added Zn-Al-Mg alloys under different cooling rates are displayed in Fig.7. According to the electrochemical theory, the corrosion potential and the corrosion current are the main factors of the corrosion resistance. Thereinto, the corrosion potential reflects the trend and possibility of the corrosion reaction, and the corrosion current reflects the practical process and kinetics of the corrosion reaction. It is generally recognized that the value of corrosion current represents the practical corrosion degree during the corrosion process. From Fig.7, it can be concluded that the water-cooled alloy samples possess the best corrosion resistance, and with the addition of B, the corrosion resistance is further enhanced. The furnacecooled alloys show the least corrosion resistance, mainly because there exist few or no TiAlparticles available for heterogeneous nucleation in the solidified microstructures, and the grain sizes are too coarse to obtain excellent corrosion resistance.

Fig.7 Polarization curves of the (a) Zn-6%Al-3%Mg-0.1%Ti and (b) Zn-6%Al-3%Mg-0.1%Ti-0.05%B as-cast alloys under different cooling rates

Fig. 8 The Nyquist curves and the fitted equivalent circuits of the (a) Zn-6%Al-3%Mg-0.1%Ti and (b) Zn-6%Al-3%Mg-0.1%Ti-0.05%B ascast alloys under different cooling rates
Based on the measurement of the polarization curves, the electrochemical impedance spectroscopy (EIS) curves were determined to further explore the mechanism of the electrochemical behavior. The Nyquist curves and the corresponding fitted equivalent circuits of the Ti/B added Zn-Al-Mg alloys are displayed in Fig.8, and the fitted parameters of the equivalent circuit components are shown in Table 3. It could be noticed that the fitted models of the Nyquist curves are similar under different cooling rate, and the furnace-cooled alloys take on slight difference on the corrosion mechanism compared with the quenched and air-cooled alloy samples, mainly due to the difference of the related surface conditions. In the equivalent circuits,R
,R
, andR
represent the solution resistance, charge transfer resistance of the double electric layer and the surface resistance respectively, andQ
,Q
represent the corresponding constant phase angle elements (CPE). The corrosion reactions include two electrochemical time constants,i e
, the charge transfer process in the double electric layer and the diffusion process between the electrode surface and the electrolyte solution. It is obvious that the quenched alloys have the maximum equivalent resistance, which means these alloy samples possess optimum corrosion resistance. The Bode plots of the Ti/B added Zn-Al-Mg alloys under different cooling rates are also displayed in Fig.9. It can be seen that in the low frequency region, the corrosion resistance arrangements in descending order should be quenched alloy>air-cooled alloy>furnace-cooled alloy, which is in consistent with the Tafel polarization curves and the Nyquist plots in Figs.7 and 8, respectively. And in terms of the quenched samples, it is suggested that the corrosion resistance of the 0.1%Ti and 0.05%B added alloy is better than that of the 0.1%Ti added alloy. It can be interpreted that under the fast cooling rate, a trace amount of B will increase the nucleation sites in the molten zinc, and the nucleation rate of the TiAlparticles is further enhanced. So it is of great significance to properly increase the cooling rate of the Ti/B added Zn-Al-Mg coatings in the actual manufacturing process.Table 3 The fitted parameters of the Ti/B added Zn-Al-Mg as-cast alloys
Composition Solidification Rs/(Ω·cm2) CPE/Y01 CPE/n1 R1/(Ω·cm2) CPE/Y02 CPE/n2 R2/(Ω·cm2)0.1%Ti Water-cool 53.68 5.16×10-6 1 77.4 7.00×10-4 3.59×10-1 1 454 0.1%Ti Air-cool 14.66 3.89×10-4 5.30×10-1 131.6 9.90×10-4 3.11×10-1 1 373 0.1%Ti Furnace-cool 16.43 1.16×10-3 4.62×10-1 50.6 5.13×10-3 5.90×10-1 940.3 0.1%Ti0.05%B Water-cool 29.32 2.21×10-4 7.26×10-1 578.6 2.40×10-3 7.01×10-1 1 894 0.1%Ti0.05%B Air-cool 14.22 2.03×10-4 5.12×10-1 442.9 3.73×10-3 9.73×10-1 82.68 0.1%Ti0.05%B Furnace-cool 16.84 6.25×10-4 5.47×101 34.3 5.18×10-3 4.63×10-1 1 104

Fig.9 Bode plots of the (a) Zn-6%Al-3%Mg-0.1%Ti and (b) Zn-6%Al-3%Mg-0.1%Ti-0.05%B as-cast alloys under different cooling rates
The solidification and the corrosion behavior of the Ti/B added Zn-Al-Mg alloys were theoretically and experimentally investigated. It is discovered that the addition of Ti/B and the increase of the solidification rate will benefit the microstructure morphologies and the corrosion resistance. The conclusions are as the following:
The precipitated temperatures and the phase categories of the Ti-added Zn-Al-Mg alloys are predicted using the thermodynamic calculations. Also, by means of DFT calculations, it is predicted that the D0-TiAlphase plays a vital role in the refinement of the grain size and the elevation of the microhardness, and the TiAl/Al interface is more stable than the TiAl/Zn interface, which interpreted the Al phase will precipitate on the TiAlparticles preferentially.
In the investigation of the microstructures of the Ti/B added Zn-Al-Mg alloy samples under different cooling rates, it could be discovered that the added Ti/B will refine the primary Al-rich phase, which is in consistence with the prediction of the DFT calculation.
The electrochemistry test results further indicate that the corrosion resistance arrangements should be quenched alloy>air-cooled alloy> furnace-cooled alloy in descending order. It could also be discovered that with the addition of B, the corrosion resistance of the quenched alloy is further enhanced possibly due to the increase of the TiAlnucleation sites in the molten zinc.
To sum up, in the composition design of the zinc pot, 0.1%Ti and 0.05%B could be added to enhance the nucleation rate of the precipitated phases of the Zn-Al-Mg coatings during the solidification process. The cooling rate could be elevated moderately in order to obtain the required surface quality and the corrosion resistance of the Ti/B added Zn-Al-Mg coatings. The present study may provide a feasible approach for the actual manufacturing process of the galvanized coatings.
Journal of Wuhan University of Technology(Materials Science Edition)
2022年4期