Influence of Na2SiO3/NaOH Ratio on Calcined Magnesium Silicate Based Geopolymer—Experimental and Predictive Study

2023-10-07 13:56:36PremkumarRameshBabuChokkalingamMeyyappanPLShanmugasundaram

Premkumar R ,Ramesh Babu Chokkalingam ,Meyyappan PL ,Shanmugasundaram M

(1.Kalasalingam Academy of Research and Education, Krishnan Koil, Tamil Nadu, 626126 India; 2.Vellore Institute of Technology - Chennai, Tamilnadu, 600127 India)

Abstract: This study aims to investigate the behavior of alkali activated mortar,which is made of naturally available magnesium silicate as source material.For magnesium silicate,ultrafine natural steatite powder (UFNSP) is used as the primary source of binder,and the activation is initiated through the alkali liquid which is proportioned in various combinations of silicate to hydroxide ratio (Na2SiO3/NaOH) ratio,and this ratio in this study varies from 1 to 3.The UFNSP is calcined at two different temperatures,700 and 1 000 ℃.The mortar mix is proportioned as 1:3 between powder and the fine aggregate,and the mortar is prepared with hydroxide molarity (M) of 10 M.The mortar is cured for 48 hours at 60 ℃ and the compressive strength was studied.All the mix were studied for its microstructural behavior along with compressive strength.The mix proportion of the mortar,and the results obtained through microstructural characterization were combinedly formed as input for artificial neural network(ANN) predictive modelling.The model is designed to predict the compressive strength,which is trained through Bayesian regularization algorithm with varying hidden neurons of 7 to 10.This experimental and predictive study shows that the strength is influenced by both Na2SiO3/NaOH ratio and calcination process.And the ANN is influenced by mainly calcination temperature and uncorrelation occurs in selected samples of 1 000 ℃ calcined UFNSP mix.

Key words: magnesium silicate;silicate;alkali activation;geopolymer;UFNSP;prediction

1 Introduction

Alkali activated binder technique (geopolymerisation) is a method where large amount of natural and industrial byproduct rich in silica and alumina,can be used as source materials and be used as an effective alternative to cement[1,2].Geopolymer is usually made of polymer chain that occurs through the presence of aluminosilicate rich geological products[3,4].The process of hardening occurs through dissolution and condensation phases.In dissolution the silica and alumina get separated from the source in presence of alkaline liquid,then slowly get hydrated,transporting its ions to form monomers.The monomers get condensed,forming amorphous gel[1,5,6].The alkali activation of silicate based materials not only improves the strength and performance,but also has environmental benefits[5,7-9].The silicate rich materials are either used as raw feed or thermally treated and used as the source of geopolymer ensuring the binding properties of the materials[5,10].

Steatite is a natural form of metamorphic hydrated magnesium silicate available in abundance in India[11],which can increase the mechanical properties of mortar and concrete[12-15].In early studies it was observed that the highest compressive strength (43 MPa) and lowest apparent porosity (0.19%) are achieved when steatite particles are coarser (ranging from 1.41 to 0.42 mm),and 40% of polymeric phase is employed[16].Also,there were studies which concentrates on steatite based composite cementitious materials used in restoration of steatite elements and the compressive strength showed good results[17].The steatite was then calcined and used as cementitious materials[18].Early studies were made on steatite as source material for geopolymer.At higher molarity of hydroxide solution and along with catalyst like polyvinyl alcohol,the compressive strength is 55 MPa[19,20].The magnesium and magnesium-based minerals are used as an alternative to calcium-based minerals in cementitious materials and binders[21,22].This magnesium based binding system provides environmental benefits and also is used in enhancing the performance of concrete and cement matrix[23,24],which also influence the microstructural behavior of mortars and concretes[25,26].

The artificial neural network (ANN) is used as an effective tool in predicting the compressive strength of various construction and building materials[27].There are many studies made on the effective model of prediction of compressive strength of alkali activated and conventional binder sourced concrete and mortars[28-32].These studies on prediction help in understanding the influencing parameters of the studies and also create a future proof design reducing the time and cost and finalizing the mix.

This study is to understand the influence of Na2SiO3/NaOH ratio on the calcined steatite.Through ANN prediction it is proposed to create a model and evaluate its performance.

2 Experimental

2.1 Materials

Naturally available hydrated metamorphic magnesium silicate (steatite) is cut into panels and grinded using ultra fine grinders,and the product from this process is ultrafine natural steatite powder(UFNSP).The physical and chemical properties of UFNSP is presented in Table 1,and this UFNSP is calcined in muffle furnace to 600 and 1 000 ℃,and this calcined UFNSP is used as the primary source material.The alkaline liquid is prepared using sodium silicate (Na2SiO3) and sodium hydroxide (NaOH).The sodium hydroxide solution is prepared for 10 molar concentrations (1 molar=40 g of flakes/ litre of neutral water),and this sodium hydroxide is prepared 24 hours before the casting process.The standard sand is used as the fine aggregate,and this standard sand is procured from TAMIN under Grade-I,Grade-II and Grade-III classification confirming to Indian standard IS650:1991.

Table 1 Properties of UFNSP

2.2 Mixing process and mix proportion

The calcined UFNSP powder (600 and 1 000 ℃)is mixed along with the standard sand under dry state in mortar mixer,then alkali liquid is slowly added to form mortar.There were ten different combinations of mixes manufactured for this study and is presented in Table 2.The mortars were casted in cube of size 70.6 mm×70.6 mm × 70.6 mm,and after 24 hours of casting the mortar cubes were kept in hot air oven for a period of 24 hours in 60 ℃.After 24 hours the mold was removed and again 24 hours 60 ℃ curing was done.It is ensured that the total curing period does not exceed 48 hours,and mortar cubes were tested.

Table 2 Mix proportion

2.3 Testing methodology

The compressive strength of mortar cubes was tested in compression testing machine (CTM) of load capacity 1 000 kN,and the test was conducted in accordance to IS:4031-Part 6-1988.The micro structure of the samples was tested through the scanning electron microscope (with energy dispersive X-ray analysis) and X ray diffraction test.For SEM and EDS the samples were cut from undisturbed mortar cubes,and for XRD the samples from mortar cubes were powdered and sieved in 90 micron sieve and used.The SEM was used to capture and analyze the hardened samples up to 1 000 magnification.The XRD analysis was carried out with X-ray diffractometer with Cu K-beta radiation and 2 scanning with a step size of 0.02° and a measuring time of 10.00 Deg/minute.A voltage of 40 kV and current of 15 mA were used.

2.4 Artificial neural network prediction and performance evaluation of the model

The prediction was carried through MATLAB R2019b.The basic architecture of ANN used in this study is shown in Fig.1.The prediction was carried out through ANN tool with two-layer feed forward network with sigmoid hidden neurons and linear output neurons.During the modelling,60% of sample was used for training and balance 40% was used for testing and validation.The training algorithm used to train the data set was Bayesian regularization algorithm(trainbr),which typically requires more time,but can result in good generalization for difficult,small or noisy datasets.Training stops according to adaptive weight minimization (regularization).The performance of the prediction model was tested through coefficient of determination (R2) calculated through scatter plot plotted in MS excel.

Fig.1 ANN architecture

3 Results and discussion

The experimental results and predictive analysis in this study are presented in Table 3,Table 4,Fig.2 and Fig.8.The study is categorized into three parts,i e,compressive strength,microstructural analysis and prediction model.The results are consolidated and discussed in detail.

Table 3 EDS and XRD results

Table 4 ANN model

Fig.2 Compressive strength of mortars with respect to Na2SiO3/NaOH

3.1 Compressive strength

The compressive strength of the mortars is tested after the samples are cured under 60 ℃ for 48 hours,and the results is presented in Fig.2.The strength can be observed in two categories,the first is based on the magnesium silicate calcination temperature and the second is based on the weight ratio of sodium silicate to sodium hydroxide which forms as alkali liquid (activators).The results show that the samples made with higher order calcined source materials show higher strength.The strength of samples with 1 000 ℃ calcined shows better compressive strength than the samples with 700 ℃ in all combinations of alkali liquids.The strength gained in 1 000 ℃ samples is 28%,16%,14%,19% and 2% higher than 700 ℃calcined samples for alkali liquid ratio of 1,1.5,2,2.5 and 3 respectively.The highest strength is observed in Mix 8 and the lowest value in Mix 1.The strength increases as the calcination temperature of source material is higher and this may be due to the higher reactive magnesia and silica which is the resultant of the calcination process.In 700 ℃ calcined group Mix 1 which has silicate to hydroxide ratio as 1 has the least compressive strength value and Mix 3,Mix 5,Mix 7,Mix 9 has 30%,55%,64%,and 34% higher strength in comparison to Mix 1.In 1 000 ℃ calcined group Mix2 which has silicate to hydroxide ratio as 1 has the least compressive strength value and Mix 4,Mix 6,Mix 8,Mix 10 has 18%,38%,53% and 7% higher strength in comparison to Mix 2.It is observed that the samples with silicate to hydroxide ratio as 2.5 has the highest strength in both the groups,and the least value is observed in samples with ratio 1.Also,the samples with ratio of silicate to hydroxide as 3 has value less than 1.5 to 2.5 and is almost near to ratio 1 samples,which shows silicate to hydroxide higher ratio might also affect the strength of the samples.The strength gain is attributed to the presence of magnesium-based products which also gives the strength enhancement similar to calcium-based products[11,13,33].Also,the ratio of sodium silicate to sodium hydroxide influences the strength gain with 2.5 as the best performing ratio similar to early studies[34].Even though the strength gain is not as high as metakaolin[35],the strength is more than that of geopolymer created with soapstone[36].Thus,calcined UFNSP can be effective in producing alkali activated building materials.

3.2 Microstructure study

The micro structure study has 3 phases on all samples.The results of these study are presented in Fig.3 to Fig.5 and in Table 3.

The SEM and EDS images of group 1 samples with 700 ℃ calcined UFNSP as source material are shown in Fig.3 and the element presence is shown in Table 3.The results show that,as the ratio of silicate to hydroxide increases the microstructure grows denser and there were more activated particles.The lower silicate to hydroxide ratio shows larger presence of unreacted UFNSP particles and as the ratio increases there is more solid and denser gel phase.The Mix 7 and Mix 9 (Figs.3(d) and 3(e)) shows the denser micro structure with the least unreacted phase and Mix 1 (Fig.3(a)) shows the larger unreacted phase with very weak micro structure.A phase change transition is observed in Mix 5 (Fig.3(c)) which has silicate to hydroxide ratio as 2.Mix 5 (Fig.3(c)) has equal presence of reacted and unreacted phases,and also shows visibility of alkali activated region containing silicate.In comparison to Mix 5,Mix 3 (Fig.3(b))shows less reacted phase,and also shows visibility of small alkali activated regions,with less silicate.The samples with silicate to hydroxide ratio from 2 to 3 shows reacted silica aka alumino-silicate products visibly over the entire region.There are very few unreacted compounds.Mix 1 and Mix 2 which has less silicate to hydroxide ratio shows traces of unreacted silica and unreacted magnesium with little reacted aluminum and silica gels.The SEM and EDS images of group2 samples with 1 000 ℃ calcined UFNSP as source materials is shown in Fig.4,and the element presence is shown in Table 3.

Fig.4 SEM and EDS images of samples prepared with 1 000 ℃sintered UFNSP

This group shows denser micro structure in less silicate to hydroxide like 1.5 (Mix 4).The least reaction is noticed in Mix 2 and denser micro structure is observed in Mix 10.The Mix 10 shows appearance of microcracks causing the huge loss in compressive strength.The micro cracks might be due to excessive reactions that happened during the process of alkali activation.Mix 2 and Mix 4 (Figs.4 (a1) and 4(b1))shows presence of unreacted compounds of silica,alumina and magnesium,but Mix 4 (Fig.4(b1)),shows presence of alkali activated products,in the central part.Mix 6 (Fig.4(c1)) shows reacted alumina and silicate.Mix 8 (Fig.4(d1) shows presence of heavier reacted magnesium in the form of silicates and oxides.A micro hole is also observed in Fig.4(d1) and this shows the activation process happened in faster pace resulting in weaker microstructure in Mix 10.The Fig.5 shows the XRD pattern and it is observed that the presence of quartz increases with increase in silicate to hydroxide ratio,and this is attributed to higher strength in high silicate to hydroxide samples.All the sample show traces of magnesium hydroxide and struvite,and these does not have great impact on strength behavior.Magnesium hydroxide has influenced the denseness in microstructure,and it is evident that Mix 7 to Mix 10 shows higher peak of magnesium hydroxide and it is directly reflected in dense bond through the microstructure.The ratio of SiO2to Al2O3can also be derived through this XRD patterns and the observation show that Mix 1,Mix 3,Mix 5,Mix 7 and Mix 9 which has 700 ℃ calcined UFNSP shows the ratio of SiO2/Al2O3as 2.08,1,1,2.00,and 3.95 respectively.Similarly,Mix 2,Mix 4,Mix 6,Mix 8 and Mix 10 which has 1 000 ℃ calcined UFNSP shows the ratio of SiO2/ Al2O3as 2.50,2.78,2.00,3.00 and 1.00 respectively.Mix 7 and Mix 8 which has the sodium silicate to sodium hydroxide ratio as 2.5 shows maximum silicate to alumina ratio in both the group and this supports the higher performance of the mortar under compression.The microstructure of alkali activated UFNSP is based on silica and alumina presence and the activation of alkali liquid[7,8,37].The samples with less silicate activators show unreacted compounds[38],but most of the higher concentration of sodium silicate shows more reaction similar to early studies[39,40],and thus the Si to OH ratio is best at 2.5.

Fig.5 XRD patterns of samples

3.3 Prediction model and its performance

The prediction is made through artificial neural network (ANN),trained through Bayesian regularization algorithm (Trainbr) and Table 4 shows the details of inputs and results observed through the predicted model.The results are also discussed through Fig.6 to Fig.8.

Fig.6 Correlation between experimental and predicted value: (a)ModelX-1;(b) ModelX-2;(c) ModelX-3;(d) ModelX-4

ModelX which has 14 inputs with hidden neurons from 7 to 10 is trained to predict the compressive strength of the alkali activated UFNSP based mortar.Based on the experimentals value inputs are strengthened in the model along with the mix proportions.The initial model shows that ModeX requires less iteration to reach the best performance than ModelY and huge variation in epoch is noted from Table 4.The strength is predicted and correlation with experimental value is plotted (Fig.6) along withR2values for understanding the performance of the model.TheR2Values of ModeX-1 to ModeX-4 is 0.561 8,0.474 7,0.563,0.680 7 respectively.The ModelX-1 and ModelX-2 (Figs.6(a) and 6(b)) has more than one uncorrelated value with experimental results,and hence this cause a huge reduction inR2values,where as in ModelX-3 and ModelX-4 (Figs.6(c) and 6(d)) the Mix with silicate to hydroxide ratio as 3 alone causes huge uncorrelation.When this uncorrelated value is removed from model ModelX-3 perform withR2value of 0.982 7 and ModelX-4 increases its performance to 0.92 as itsR2value.

The error values are observed in 2 groups,Mix with 700 ℃ calcined UFNSP and 1 000 ℃ calcined UFNSP.In group1 (Fig.8(a)) the models with 9 and 10 neurons have steady error values and no deviation is observed.While as models with 7 and 8 neurons show huge variation in errors.In group 2 (Fig.8(b))the least errors were observed in Mix4 and huge errors are observed in Mix10 in models with 9 and 10 hidden neurons.The ModelY series was formed with 8 inputs including mix proportion and SiO2to Al2O3ratio (XRD),and the prediction was carried with Trainbr with 7 to 10 hidden neurons.The predicted values are plotted(Fig.7) along with experimental value andR2values are observed,to understand the performance of the model.TheR2value of ModelY-1 to ModelY-4 is 0.523 3,0.467,0.525 and 0.480 respectively.The correlation coefficient is low when compared with ModelX but it is observed that the correlation is highly affected by only one mix (Mix10).Contrary to ModelX,all the ModelY were affected by Mix10 and when it is removed from the created model,ModelY-1 to ModelY-4 performance can be increased to 0.958 1,0.951 5,0.879 2 and 0.953 6 respectively.With Mix10,ModelY-3 (Fig.7(c))performance to maximum correlation.The error values of mix were grouped in 2 categories,group1 with 700℃ and group2 with 1 000 ℃ calcined UFNSP material,and the error values (Figs.8(c) and 8(d)) shows that MIX10 has the highest difference in predicted value in comparison with experimental value.In group1 all the models in Mix1(Fig.8(c)) have minimum error values.In group2 (Fig.8(d)) Mix2,Mix4 and Mix6 has minimum error values,which is almost nil.After analyzing ModelX and ModelY the performance of ModelX performs higher than ModelY and also there is huge uncorrelation created by Mix10.

Fig.7 Correlation between experimental and predicted value: (a)ModelY-1;(b) ModelY-2;(c) ModelY-3;(d) ModelY-4

Though the performance of the models is less than the early studies[41-44],the strength prediction shows good results,and this model performance is affected by only one Mix and after removing the noisy sample[45-47]more precise result can be achieved.This study shows that inclusion of XRD and EDS values will strengthen the ANN model and the neurons for this study can be fixed as 9 as most of the results are correlated in this model.The models can be further strengthened in further studies through the inference presented in this study.

4 Conclusions

a) The strength of the mortar is influenced by the Na2SiO3/NaOH ratio and the calcination process.The strength increases with the increase in silicate to hydroxide ratio,and the maximum value is achieved in ratio of 2.5.Also,the strength increases with higher calcination temperature.All specimens of 1000 ℃calcined UFNSP based mortars shows higher strength gain when compared with 700 ℃ UFNSP as source materials.

b) The strength gain in this study is attributed to formation of reacted magnesium,silicate and aluminum phase,and denser microstructural appearance.The calcination has induced more reactive amorphous compounds,which in turn had given strength to the alkali-activated mortars.

c) Even though Na2SiO3/NaOH ratio influences the strength gain,at the ratio of 3 there is a higher strength loss in both cases of calcined UFNSP,and this is due to the faster reaction and week micro structure.The influence of silicate is evident in the alkaliactivated UFNSP mortar,and when the ratio reaches 2.5 to 3 the strength performance of the mortar is relatively high,due to the influence of Si and Al in strength gain of mortar.

d) The ANN model performance is related to the inputs used to create the model.The models with EDS and XRD values along with basic mix proportion performs good than with models with only mix proportion and SiO2/Al2O3ratio as input.Also the mix with silicate to hydroxide ratio of liquid as 3 causes huge uncorrelation in the model,which in turn affects the performance of the model.Hence the model can be further strengthened with the use of EDS and XRD observations for better performance.

e) Through the experimental and predictive study,it is found that 1 000 ℃ of calcination temperature and Na2SiO3/NaOH ratio of 2.5 is the optimum suited mix for steatite based geopolymer phenomenon for alkaliactivated UFNSP mortar

Conflict of interest

All authors declare that there are no competing interests.


登录APP查看全文